How to Test UV Flexo Ink Adhesion on Label Film

Test UV flexo ink adhesion on label film by running a candidate roll next to a film that already works on your press. Use the same ink, anilox and curing setup. Compare samples printed at production speed using the tape method agreed before the trial. Be sure to include the densest area of the art to help catch any cure issues.

When a test patch fails, keep the sample and the used test tape together. What comes away on the tape will indicate which interface to examine. You can then repeat the test under controlled conditions to determine if changing the print surface, curing conditions or test setup makes a difference.

Why UV Flexo Ink Lifts From Film

Three tape failure interfaces to inspect before changing settings (ASTM F2252/F2252M-25).

UV flexo ink can lift because it failed to adhere to the print surface, because the ink layer itself split, or because a coating separated below it. Use the ASTM tape practice for applicable flexible packaging, then inspect the sample and tape under good light to choose the next check.

Assume a new clear polypropylene roll stock comes in and the whole image lifts cleanly from the first label. If the old roll passes in the same shift using the same ink, the team can check the print side and treatment of the new roll before adjusting lamp settings. Photograph the test sample before and after pulling the tape, and label and date both the sample and the tape. If both rolls fail, confirm the result before changing the ink, curing conditions or tape procedure.

Even color can mask poor UV ink adhesion, so assess the adhesion of UV ink with the agreed tape test. Poor adhesion often first shows up in a downstream operation such as handling, laminating or rewinding. An adhesion problem on a single roll calls for a different comparison from one that accompanies the ink across all the material.

Choose the Film Surface Before the Trial

Identify the printable face, grade and wetting before testing ink adhesion (ASTM D2578-23).

Determine the printable face and actual film grade and then evaluate wetting. Biaxially oriented polypropylene (BOPP) and polyester (PET) can be provided with different print surfaces. Roll labels, winding direction and the supplier data sheet need to be in agreement regarding which side is in contact with the plate.

ASTM D2578-23 measures wetting tension of polyethylene and polypropylene films. Testing on the print side must use a consistent method, with the reading recorded alongside the roll identity and the time of measurement. Enercon’s treatment guide explains why storage and contamination can change the result.

Fresh treatment can enhance ink adhesion when poor wetting limits transfer to the film. This also affects how a given test liquid wets low surface energy materials. In shop language, surface energy refers to the solid and surface tension refers to the liquid. A wetting tension reading is obtained using a specified procedure and a test liquid.

In a laboratory study by Seidelmann and colleagues, plasma-treated BOPP supplied by study participant Innovia Films read 42 to 46 mN/m with dyne pens, yet the tape pull removed about 90% of the tested Sericol JD UV flexographic ink. That study used a specific nitrogen plasma treatment, ink and test setup. The results from the dyne test and printed tape deserve to be in separate fields of the trial record.

When to Use a Corona-Treated or Topcoated Film

Check corona eligibility or trial the topcoated grade specified by the ink maker (Enercon).

To increase wetting, use corona treatment if the film grade permits it. If the ink maker specifies a topcoated grade or the corona-treated grade repeatedly fails the agreed adhesion check despite verified curing, trial a topcoated film qualified for the ink. A print topcoat gives a different surface to the UV ink on the plastic film, so a topcoated grade needs to be qualified for print quality and adhesion as a separate construction.

For UV rather than solvent ink applications, use the film’s treated or coated face and apply inline corona treatment only where the grade permits it. When a roll performs differently after storage, compare a retained reference with a fresh candidate strip using the same ink laydown and cure. Where a grade permits bump treatment, compare treated and untreated trial strips before releasing the roll.

Film and ink compatibility matters more than choosing the right reading from a generic chart. Some inks are specifically designed for coated films. Substitutes should match the intended film surface and UV light source. UV flexo and digital printing use different transfer processes, so use a flexographic approval for this trial. If the supplier suggests adhesion promoters, test its specified formulation separately before changing the regular printing process.

Run a Controlled UV Flexo Press Trial

Hold ink and press setup constant, then track production speed and retain the reference swatch.

The printer runs the approved reel first, then substitutes the candidate without changing the ink or press setup. Print a solid, a fine detail area and the heaviest ink build on the job. Keep any varnished or laminated finish that the customer will receive, using separate samples to identify which layer changes the result. If the control fails, resolve the process or testing problem before judging the candidate.

Keep printing speed and the substrate type on the trial sheet. A sample of better adhesion after modifying several inputs can be a good production trial; however, it doesn’t tell you which modification improved the result.

Matched reference and candidate run record
Record category Approved reference Candidate film
Material Known good film grade, lot and print side New grade and lot, coating or treatment, print side and wetting reading
Ink and transfer Approved ink series, batch and anilox settings Same ink, batch, anilox and test artwork for the first run
Web treatment and cure Treater setting, lamp type, meter band, peak irradiance, dose and speed Record actual values at setup and production speed, including any change to treatment
Sample position Record press station and cross-web location Use corresponding positions and identify any edge-only or center-only failure
Opaque patch Retain the approved white or other high-coverage patch Record any loss separately from other colors and fine detail
Sampling time Record print time and agreed test interval Compare samples conditioned and tested at the same interval
Tape and method Record method revision, tape lot, application and release procedure Keep consumables and procedure the same unless the test itself is under investigation
Finish and rewind Keep bare and finished approved strips if finish affects the job Record visible transfer or blocking on the rewind, and isolate finishing from print
Disposition Keep the approved swatch and baseline result Record repeat result, next step and person responsible for release

Mark samples with speed and print station as they come off the web. Keep samples from normal production speed and, if there’s a variation on the roll, identify where each sample is from. If the art work requires white to mask a dark background, evaluate the sample to determine if it successfully masked the background. For an overlabel job, use the blockout label opacity guide to check whether old print shows through.

Check Cure at Production Speed

Record web treatment, irradiance and dose when changing line speed (Phoseon).

Check curing at the speed you’ll run, especially if opaque white holds in setup and lifts after acceleration. With the same light profile, a faster web spends less time under the lamp. Phoseon distinguishes peak irradiance, which is measured as power per area, from dose which is measured as energy per area. Compare measurements using an instrument suited to the source’s spectral band.

When you change web speed check what happened to both the inline treatment and measured UV exposure. Hold the anilox and ink fixed while comparing the reference and candidate. If the press setup permits, repeat the comparison with surface treatment held constant. If both inputs varied, the result describes the job at that speed. Use another comparison to isolate the cause.

Ink laydown, lamp output and time under the ultraviolet source are key factors affecting cure in this comparison and factors that affect the result at a new press speed. Lamp output and the chemistry of the ink influence the curing process. Ink viscosity and anilox transfer can affect ink adhesion indirectly by modifying the amount of printing ink that reaches the web. Hold the other inputs stable and compare film lots.

The data sheet for Flint Group’s EkoCure F shows how specific ink makers’ tests can be. Its example used 395 nm FirePower lamps rated at 16 W/cm² on a Mark Andy 4150 press. Record your ink series, lamp and meter readings. Published lamp ratings describe lamp and hardware configurations. To select the right ink, understand how the ink series is qualified on your UV source. Conventional UV inks may have different spectral requirements compared to some LED formulations. A surface that feels dry can still need a cure check to determine if ink is fully cured.

Agree on the Ink Adhesion Test Before Printing

Agree on the tape, pressure and pull procedure before evaluating ink adhesion (ASTM F2252/F2252M-25).

FTM 21 and FTM 22, listed by FINAT, are the basic and advanced methods of ink adhesion tests, respectively. Agree which method and version will apply, and then use the entire procedure. A pressure-sensitive adhesive peel test measures the force needed to peel a label from a specified test substrate.

ASTM F2252/F2252M-25 describes tape evaluation of ink or coating adhesion on flexible packaging surfaces that tolerate tape application and removal. The user and producer set an acceptance standard together and can improve repeatability by controlling test variables such as application pressure, pull angle and speed. Before the trial, document the acceptable patch appearance, conditioning, tape selection, application pressure, contact time, pull angle and speed for the agreed test method. Before the trial, specify any additional rub, scratch or wet exposure checks required for the finished label.

For proper adhesion, compare the newest print to the approved print using the documented tape test. Note where each patch was sampled. The same piece can show acceptable adhesion of the ink in one patch and lifting in a denser solid. To improve ink adhesion, use the location and appearance of the failure to determine the next controlled change.

Read the Tape Test and Locate the Failure

Clean film, residues on both faces or a lifted clear layer identify the next diagnostic check.

Repeat tests with unexpected results on fresh, equivalent areas of each film roll using fresh tape from the same lot to confirm or clarify the findings. If applying or removing tape damages the film, review whether the film meets the surface requirements of ASTM F2252/F2252M-25 before interpreting the ink adhesion result. Compare what transferred to the tape with what remains on the film.

Tape result and next press check
Observation First check Next comparison
Clean film under lifted color Printable face, contamination and film grade Run both films with the approved ink, then isolate a compatible treatment change
Smear or ink residue on both faces Ink film thickness, curing output or ink cohesion Compare actual dose at the same speed and check the dense solid independently
Clear layer visible with the color Whether a topcoat, primer or varnish moved Compare unvarnished and finished strips, or inspect an unprinted control from the same reel
Only high-opacity white lifts Compare white and ordinary solids at the same station and speed Keep the ink and anilox fixed while testing the cure response
Clean bands near one edge Confirm where on the web the band came from Repeat at the same cross-web positions and check treatment and lamp uniformity separately
Poor laydown before cure Inspect the printable face and wetting Compare unprinted reference and suspect film under the same wetting test
Coating appears on the unprinted control tape Check the stock surface and whether the tape damages it Hold the stock and agree an appropriate procedure before classifying ink adhesion
A pass at setup speed but failure at target speed Record treatment and cure at both settings Rerun with the treatment held constant where the press permits
Both films fail the same way Tape condition, technique, ink transfer and lamp setup Repeat with a retained approved swatch before rejecting the new reel

A pass on an immediate tape test clears the agreed upon adhesion check at that interval. If labels will be rubbed wet or stored in a cold environment, hold a separate set for the durability checks. That also helps to keep a failure during a later packaging qualification from being mistakenly called a press rejection.

Maintain acceptable adhesion on the film surface, and retain the settings that achieved it. Track curing speed and treatment separately if the production line is running at different speeds. The approved film and settings should meet the same adhesion requirements throughout the run.

Approve the Film for Production

Retain the approved film and settings before accepting a new production roll (Guanma).

Approve the particular film, ink and production conditions that passed. When a cheaper roll only passes below normal press speed, record the speed that passed and consider the extra press time and the risk of reel changes before purchasing. Hold a new lot for a trial when the print-side construction, ink or curing equipment changes and the existing approval no longer covers it. The label stock change control guide describes how to record and approve changes.

Ask about a small trial roll before putting in a production order. Confirm availability and roll size. Guanma lists BOPP and PET among its self-adhesive film constructions. See the BOPP film selection guide for grade and construction differences. The PET label stock page provides an introduction to PET constructions. Send the film grade, print side, roll width, required speed, exact UV ink and tape procedure when requesting a sample. Let them know what happened to the reference and candidate samples and the finish of the label.

Ask Guanma About a Trial Roll

The findings will help you select a suitable grade of film and identify which conditions would need to be reassessed if the film construction is changed.

Frequently Asked Questions

Which film substrates are suitable for UV printing?

Suitable films are those approved by the ink supplier for the selected UV flexo ink series and curing equipment. A treated polypropylene reel and a coated polyester reel may require different print surfaces or ink recommendations. Verify the print side before loading either roll. Run the chosen combination at production speed and include the dense areas before approving it.

What can cause ink to peel off on tape?

A tape failure can come from the ink layer or from one of its interfaces. Look at both faces. Clean film under a flake points toward the ink-to-film interface. Pigment on both faces can indicate splitting in the ink, while a clear layer on the tape points toward a coating. Compare the control and retest one changed condition.

What is the role of curing in UV printing?

UV exposure cures the deposited ink using a light source suited to the ink formulation. The amount of energy the ink receives depends on output and exposure time. The ink needs enough exposure to bond effectively to the printable surface. A print made slowly during setup may get a different dose from one run at production speed. Record the conditions and check the heaviest ink coverage at the speed you intend to use.

When should I use inline corona?

Use inline corona when the film maker permits it and you want to test whether fresh treatment will improve adhesion. Compare the treated and untreated samples under the same conditions.

What should I retain from a successful trial?

Keep a labeled swatch with the reel, ink series and lot, anilox, treatment, lamp and speed. Include the test protocol, sample location, conditioning and photographs. Keep an approved sample accessible to inspection and production so a later roll can be compared against the conditions that passed. Store the photos under the same sample identifier as the swatch, and label which side of the tape was applied to the patch.

References & Sources

WHY WE WRITE THIS
About Guanma

Guanma is a self-adhesive film, label stock, and release liner manufacturer for industrial labeling applications. Our team works with PET film, PP synthetic paper, coated paper, hot-melt PSA, acrylic PSA, water-based adhesive, glassine liner, and CCK release liner.

We write these guides to help label converters, packaging buyers, and industrial procurement teams choose materials by real application conditions instead of generic catalog names. Most label failures come from a mismatch between facestock, adhesive, liner, substrate, temperature, printing method, or end-use environment. Our content explains those decisions in practical terms.

Our Experience

Guanma’s material guidance is based on coating, lamination, slitting, sample validation, and customer troubleshooting experience across Thailand and Vietnam production. We focus on common industrial label problems such as cold-temperature peel, oil and chemical exposure, UV aging, print durability, release force, MOQ, lead time, and substrate-matched testing.

Our Expertise

We reference practical testing logic and recognized label-industry standards, including FINAT FTM peel and shear methods, ASTM peel testing methods, FDA 21 CFR 175.105, REACH, RoHS, FSC, and ISO 9001-related quality control. For custom label stock, we always recommend testing samples on the buyer’s real substrate before full production.

SYS.PROFILE
Contact Profile
Name Guanma Manufacturing Team
Brand Name Guanma
Country Thailand + Vietnam Production
Model B2B / Wholesale / Custom Coating
Main Products Self-Adhesive Film, Label Stock, Release Paper & Liner
Contact Submit RFQ via Website Form
Website https://guanmalabel.com/
Visit Website